Concrete paver blocks are widely used for parking areas, footpaths and walkways, but their production consumes large quantities of cement and natural aggregate. This paper investigates paver blocks in which part of the fine aggregate is replaced by vulcanized crumb rubber obtained from waste tyres, with styrene–butadiene rubber (SBR) latex added as a polymer modifier to improve matrix bonding. Blocks were batched, mixed, moulded, water-cured, and tested for compressive strength at 7 and 14 days and for water absorption. The average compressive strength was 11.56 N/mm² at 7 days and 12.84 N/mm² at 14 days, an increase of about 11%. The 28-day strength, projected from the 7- and 14-day trend, is about 14.12 N/mm²; this is an estimate and not a measured value. Water absorption was 0.19%. The strength is well below the 30 N/mm² minimum grade of IS 15658, so the present mix is suited only to non-load-bearing uses unless further optimized. The material cost of the batch was about Rs. 727. The work supports SDG 9, 11, 12 and 13 by turning waste tyres into a construction product.
Introduction
The study focuses on developing eco-friendly concrete paver blocks by partially replacing conventional aggregates with waste tyre crumb rubber and adding Styrene-Butadiene Rubber (SBR) latex. Conventional concrete paver blocks consume large amounts of cement and natural aggregates. Using waste materials helps reduce environmental impact and promotes recycling.
Crumb rubber improves flexibility, toughness, impact resistance and skid resistance but reduces compressive strength because of poor bonding with cement paste. To overcome this weakness, SBR latex is added to improve bonding, flexibility, water resistance and crack resistance.
1. Objectives
To determine the physical properties of the materials.
To develop suitable mix proportions for paver blocks.
To evaluate compressive strength at different curing ages.
To identify the optimum crumb rubber replacement percentage.
To compare the developed paver blocks with conventional concrete paver blocks.
2. Materials Used
Cement
Fine aggregate (sand)
Silt
Vulcanized crumb rubber from waste tyres
SBR latex
Water
3. Experimental Methodology
The materials were accurately weighed and mixed in the required proportions. Crumb rubber was added to the dry ingredients, followed by SBR latex and water. The prepared mixture was poured into paver-block moulds, compacted, demoulded and water-cured.
The blocks were tested for:
Compressive strength at 7 and 14 days.
Water absorption after drying and saturation.
4. Results and Discussion
Compressive Strength:
Curing Age
Compressive Strength
7 days
11.56 N/mm²
14 days
12.84 N/mm²
28 days
14.12 N/mm² (estimated)
The compressive strength increased by approximately 11% between 7 and 14 days due to cement hydration. The 28-day strength was projected mathematically and still requires experimental confirmation.
Water Absorption:
Dry weight: 2595 g
Saturated weight: 2600 g
Water absorbed: 5 g
Water absorption: 0.19%
The blocks showed very low water absorption, indicating good resistance to water absorption under the test conditions.
5. Comparison with IS 15658
According to IS 15658, the minimum M30 grade requires a 28-day compressive strength of 30 N/mm² and average water absorption within 6%.
Water absorption: The developed blocks satisfy the specified limit.
Compressive strength: The projected strength of 14.12 N/mm² is below the required 30 N/mm².
Therefore, the tested blocks do not qualify as standard M30 concrete paving blocks.
6. Cost Analysis
The estimated material cost per batch is approximately ?727.
SBR latex: ?377
Cement: ?350
Sand, silt, crumb rubber and water: Considered free.
SBR latex is the major contributor to the overall material cost.
Conclusion
Paver blocks with crumb rubber and SBR latex were cast and tested. Average compressive strength rose from 11.56 N/mm² at 7 days to 12.84 N/mm² at 14 days, and the 28-day strength is projected at about 14.12 N/mm². Water absorption was 0.19%, and the batch cost was about Rs. 727. The blocks are well below the IS 15658 minimum strength, so this mix is a preliminary result suited only for non-load-bearing uses.
Future work should: (i) test the blocks at 28 days and replace the projected value; (ii) test more blocks per age; (iii) vary crumb rubber (0–20%) and SBR dosage to find the optimum mix; (iv) add fly ash, marble waste, red mud, silica and fibreglass; (v) measure flexural strength, abrasion resistance, density and impact resistance; and (vi) compare against a control mix without waste materials.
References
[1] H. M. Mohamad, “Manufacture of concrete paver block using waste materials and by-products: A review,” Int. J. GEOMATE, vol. 22, no. 93, 2022, doi: 10.21660/2022.93.J2363.
[2] B. M. Rethinavelsamy and C. Natarajan, “Investigation on precast concrete paver block with waste tyre crumb rubber,” Road Mater. Pavement Des., vol. 17, no. 3, pp. 719–736, 2016, doi: 10.1080/14680629.2015.1119056.
[3] S. He, Z. Jiang, H. Chen, Z. Chen, J. Ding, H. Deng, and A. S. Mosallam, “Mechanical properties, durability, and structural applications of rubber concrete: A state-of-the-art review,” Sustainability, vol. 15, no. 11, p. 8541, 2023, doi: 10.3390/su15118541.
[4] S. Gamage, S. Palitha, D. P. P. Meddage, S. Mendis, H. M. Azamathulla, and U. Rathnayake, “Influence of crumb rubber and coconut coir on strength and durability characteristics of interlocking paving blocks,” Buildings, vol. 12, no. 7, p. 1001, 2022, doi: 10.3390/buildings12071001.
[5] R. B. Ataria and Y. C. Wang, “Mechanical properties and durability performance of recycled aggregate concrete containing crumb rubber,” Materials, vol. 15, no. 5, p. 1776, 2022, doi: 10.3390/ma15051776.
[6] H. Liu, X. Wang, Y. Jiao, and T. Sha, “Experimental investigation of the mechanical and durability properties of crumb rubber concrete,” Materials, vol. 9, no. 3, p. 172, 2016, doi: 10.3390/ma9030172.
[7] M. R. Ashraf, U. Akmal, N. Khurram, F. Aslam, and A. F. Deifalla, “Impact resistance of styrene–butadiene rubber (SBR) latex-modified fiber-reinforced concrete: The role of aggregate size,” Materials, vol. 15, no. 4, p. 1283, 2022, doi: 10.3390/ma15041283.
[8] M. Kligys and G. Girskas, “Styrene–butadiene rubber latex modified mortars prepared with high early strength Portland cement,” Materials, vol. 17, no. 23, p. 6000, 2024, doi: 10.3390/ma17236000.
[9] A. El-Zohairy, M. Sanchez, B. Abediniangerabi, and P. Moler, “Performance of rubberized concrete and the effect of temperature and stainless steel fibers,” Buildings, vol. 13, no. 2, p. 280, 2023.
[10] Y. Li, J. Chai, R. Wang, Y. Zhou, and X. Tong, “A review of the durability-related features of waste tyre rubber as a partial substitute for natural aggregate in concrete,” Buildings, vol. 12, no. 11, p. 1975, 2022, doi: 10.3390/buildings12111975.
[11] F. Duan, H. Zhu, Y. E. Ibrahim, and M. Adamu, \"Durability and property study of decade-old crumb rubber concrete cored specimens,\" Materials, vol. 15, no. 16, p. 5490, 2022, doi: 10.3390/ma15165490.
[12] A. Grinys, M. Balamurugan, A. Augonis, and E. Ivanauskas, “Mechanical properties and durability of rubberized and glass powder modified rubberized concrete for whitetopping structures,” Materials, vol. 14, no. 9, p. 2321, 2021, doi: 10.3390/ma14092321.
[13] P. Kara De Maeijer, B. Craeye, J. Blom, and L. Bervoets, “Crumb rubber in concrete—The barriers for application in the construction industry,” Infrastructures, vol. 6, no. 8, p. 116, 2021, doi: 10.3390/infrastructures6080116.
[14] D. A. Singaravel, P. Veerapandian, S. Rajendran, and R. Dhairiyasamy, “Enhancing high-performance concrete sustainability: Integration of waste tire rubber for innovation,” Sci. Rep., vol. 14, Art. no. 4635, 2024, doi: 10.1038/s41598-024-55485-9.
[15] E. Mohseni and M. Koushkbaghi, “Recycling of landfill waste tyre in construction materials: Durability of concrete made with chipped rubber,” Constr. Build. Mater., vol. 409, Art. no. 134114, 2023, doi: 10.1016/j.conbuildmat.2023.134114.
[16] O. Na and G. Lee, “Mechanical and durability properties of rubberized sulfur concrete using waste tire crumb rubber,” Materials, vol. 17, no. 21, p. 5269, 2024, doi: 10.3390/ma17215269.
[17] Y. Daou and J. J. Assaad, “Use of SBR latexes to mitigate inferior concrete properties resulting from recycled coarse aggregates,” Int. J. Civil Eng. Technol., vol. 7, no. 3, pp. 67–80, 2016.
[18] X. Zhou et al., “Research on the fracture properties and modification mechanism of polyester fiber and SBR latex modified cement concrete,” Adv. Mater. Sci. Eng., vol. 2016, Art. no. 5163702, 2016.
[19] A. Bhogayata and N. K. Arora, “Workability, strength, and durability of concrete containing recycled plastic fibers and styrene-butadiene rubber latex,” Constr. Build. Mater., vol. 180, pp. 382–395, 2018, doi: 10.1016/j.conbuildmat.2018.05.175.
[20] P. Palson, “Strength and durability of styrene-butadiene latex modified concrete,” J. Civil Eng. Technol., vol. 5, no. 1, pp. 1–9, 2018.
[21] B. M. Rethinavelsamy and C. Natarajan, “Investigation on the use of waste tyre crumb rubber in concrete paving blocks,” Comput. Concr., vol. 20, no. 3, pp. 311–318, 2017, doi: 10.12989/cac.2017.20.3.311.
[22] M. Sambucci and M. Valente, “Ground waste tire rubber as a total replacement of natural aggregates in concrete mixes: Application for lightweight paving blocks,” Materials, vol. 14, no. 24, p. 7493, 2021, doi: 10.3390/ma14247493.
[23] A. K. Chaurasia, S. Gupta, V. Kumar, and A. Goel, “Effect of tyre waste on ground granulated blast furnace slag (GGBFS) based concrete blocks,” Indian J. Sci. Technol., vol. 15, no. 35, pp. 1732–1737, 2022, doi: 10.17485/IJST/v15i35.1101.
[24] T. Sembiring and C. P. Harahap, “Utilization of polypropylene plastic waste, used rubber tire and fly ash as raw materials of paving block,” AIP Conf. Proc., vol. 2221, 2020, doi: 10.1063/5.0003789.
[25] A. O. Mashaly, B. A. El-Kaliouby, B. N. Shalaby, A. M. El-Gohary, and M. A. Rashwan, “Effects of marble sludge incorporation on the properties of cement composites and concrete paving blocks,” J. Clean. Prod., vol. 112, pp. 731–741, 2016, doi: 10.1016/j.jclepro.2015.07.023.
[26] M. Meera, B. Durga Vara Prashad, and S. Gupta, “Experimental investigations on concrete with fly ash and marble powder for paver blocks,” Int. J. Eng. Technol., vol. 7, no. 3.32, pp. 120–122, 2018, doi: 10.14419/ijet.v7i3.32.18410.
[27] R. Siddique, G. Kaur, and M. Singh, “Determination of mechanical properties and environmental impact due to inclusion of fly ash and marble waste powder in concrete,” Structures, vol. 25, pp. 613–630, 2020, doi: 10.1016/j.istruc.2020.03.040.
[28] M. Hamza et al., “Evaluation of mechanical properties of paver blocks by replacing cement with fly ash and marble waste,” Discover Appl. Sci., vol. 6, Art. no. 221, 2024.
[29] K. Viyasun, R. Anuradha, K. Thangapandi, D. Santhosh Kumar, A. Sivakrishna, and R. Gobinath, “Investigation on performance of red mud-based concrete,” Mater. Today: Proc., vol. 39, no. 1, pp. 796–799, 2021, doi: 10.1016/j.matpr.2020.09.637.
[30] C. B. Truong, \"Study on fly ash-based interlocking concrete paver block using chopped fibers,” IOP Conf. Ser.: Mater. Sci. Eng., vol. 988, Art. no. 012060, 2020, doi: 10.1088/1757-899X/988/1/012060.
[31] S. Bressi, N. Fiorentini, J. Huang, and M. Losa, “Crumb rubber modifier in road asphalt pavements: State of the art and statistics,” Coatings, vol. 9, no. 6, p. 384, 2019, doi: 10.3390/coatings9060384.
[32] O. Guerrero-Bustamante, R. Camargo, I. Dawd, et al., “Implementation of crumb rubber (CR) in road pavements: A comprehensive literature review,” Infrastructures, vol. 9, no. 12, p. 223, 2024, doi: 10.3390/infrastructures9120223.
[33] Bureau of Indian Standards, Precast Concrete Blocks for Paving — Specification, IS 15658:2006, New Delhi, India, 2006.